Back to document page

lamination. c. Prepreg with lower surface resin (ie 7628). d. Control of etch-back process. Corrective Action 1. Control the oxide chemistries. 2. Use adequate hot and deionized water rinses in oxide line. (Critical!) 3. Control lamination press cycle within manufactures recommendations. 4. Use prepreg selections (against copper details) which have